TCR Engineering stress-rupture tests ASTM A453 Grade 660 bolting to ASTM E139 at its Mahape laboratory in Navi Mumbai, under NABL certificate NABLT0726MH18640, at the specification's condition of 650 °C and 385 MPa. It is an acceptance test with two traps: the bar carries a notch that can fail the lot outright, and it runs to rupture, not to a clock.
- Material: ASTM A453 Grade 660, an iron-base austenitic alloy of the A-286 type (UNS S66286), hardened by ageing, used for high-temperature bolting.
- When the test applies: clause 8.2.1, for bolting with a design temperature above 800 °F [427 °C]. Untested material is stamped NR; Grade 660 Class D and Grade 668 are exempt and stamped NR.
- Test condition: 650 °C at 385 MPa, with a minimum time to rupture of 100 hours, from Table 6 of the specification.
- Specimen: a combination smooth and notched bar to Fig. 1 and Table 7, from an 18 mm × 18 mm × 250 mm blank.
- Acceptance: rupture in the smooth section, after at least the minimum time, with at least the minimum elongation in Table 6.
- After the minimum time: stress may rise 34.5 MPa (5,000 psi) every 8 to 16 hours until rupture.
- On the NABL scope: creep and stress rupture to ASTM E139, with elongation and reduction in area as the accredited stress-rupture parameters, and time-for-rupture notch tension tests to ASTM E292.
What clause 8.2 of ASTM A453 actually asks for
Clause 8.2 of ASTM A453 is short, and almost every sentence in it changes how the test is run. A fastener manufacturer in the Gulf recently asked TCR Engineering for this test on Grade 660 bolting, and asked whether the laboratory is ISO/IEC 17025 accredited for stress rupture, whether ASTM E139 is in its scope, and whether it has the equipment for the temperature and load. All three answers were yes. The real decisions sit in the clause:
| Clause | What it says | What it means at the test bench |
|---|---|---|
| 8.2.1 | Bolting for design temperatures above 427 °C meets Table 6; untested material is stamped NR; Class D and Grade 668 exempt | Class and design temperature decide whether a test is owed |
| 8.2.2 | As many specimens as tension specimens | The count follows the tension test plan |
| 8.2.3 | Same location and orientation as tension specimens | The rupture bar comes from where the tension bar does |
| 8.2.4.1 | Test to Practice E139 | Temperature, loading and measurement follow E139 |
| Note 1 | Fig. 1 specimen taken from E292, only to detect notch sensitivity; E292 data not reported | The notch is a detector, not an E292 test |
| 8.2.4.2 | Combination bar, continued to rupture, rupture in the smooth section | One bar answers life and notch behaviour |
| 8.2.4.3 | With purchaser approval, separate smooth and notched bars from adjacent sections | Needs the purchaser's consent |
| 8.2.4.4 | After the minimum time, stress may rise 34.5 MPa every 8 to 16 hours, preferably 8 to 10 | Permitted, not required; its settings are a choice |
The NR stamp keeps untested bolting traceable: a stud stamped NR has not demonstrated the Table 6 rupture properties, so it does not satisfy clause 8.2.1 for a design temperature above 427 °C.
Why a rupture bar for bolting carries a notch
A bolt is a notched component. Every thread root is a stress concentration, and at high temperature some alloys lose rupture life at a notch faster than in a plain section. A smooth bar alone cannot reveal that notch sensitivity: it can pass its 100 hours while the same material would rupture at the thread root in service.
The combination bar puts a smooth gauge section and a notched section on one specimen, under one load. In a notch-strengthened material the constraint at the notch root delays rupture there, so the smooth section breaks first; in a notch-sensitive material the notch breaks first. Clause 8.2.4.2 makes that the test: rupture must occur in the smooth section. A notch failure does not meet the clause, however many hours the bar lasted.
Notch behaviour in an age-hardened alloy follows the condition its heat treatment produced, so the test is run on the material supplied, not taken on trust from the grade. Low rupture ductility and notch sensitivity tend to travel together, which is why the minimum elongation in Table 6 sits beside the time requirement.
Clause 8.2.4.3 allows a second route, with the purchaser's approval:
| Combination bar (8.2.4.2) | Separate smooth and notched bars (8.2.4.3) | |
|---|---|---|
| Purchaser approval | Not needed | Needed |
| Source | One bar, machined to Fig. 1 and Table 7 | Adjacent sections of the same piece, gauge sections to Table 7 |
| Run to rupture | Yes | Smooth bar, yes; notched bar need not be |
| Acceptance on the notch | Rupture occurs in the smooth section | Notched bar does not rupture in less time than its companion smooth bar |
The bar is machined in TCR's own machine shop, so the enquiry gives a blank size, not a finished bar.
A test that ends at rupture, not at 100 hours
The 100 hours in Table 6 is a minimum, not a duration. The bar must survive at least 100 hours at 650 °C under 385 MPa, and is then continued to rupture, because rupture location and elongation are part of acceptance. A sound lot may stand at 385 MPa well beyond 100 hours, and nobody knows at the start by how much.
Clause 8.2.4.4 is the answer: once the minimum time is achieved, the stress may be raised in steps of 34.5 MPa at intervals of 8 to 16 hours, preferably 8 to 10. Rupture location and elongation requirements still apply in full.
| Phase | Stress | Time at stress | What it demonstrates |
|---|---|---|---|
| Constant stress | 385 MPa at 650 °C | At least 100 hours | The Table 6 time requirement |
| Each step, if used | 419.5 MPa, then 454 MPa, and so on | The agreed interval, 8 to 16 hours | Nothing new on time; it brings the bar to rupture |
| Rupture | Whatever stress is acting | Total time recorded | Rupture location, elongation, reduction in area |
Two consequences follow. The programme length cannot be fixed in advance: it is a known minimum plus an unknown tail, confirmed in the quotation as exactly that. And a time to rupture reached under step loading is acceptance evidence for that lot, not a constant-stress rupture life; it cannot go on a Larson-Miller plot. Life prediction from creep testing of high-temperature alloys, including the accelerated tests that feed remaining life assessment, is a different programme with a different loading rule.
Why the step stress and interval are agreed before the furnace is loaded
Clause 8.2.4.4 says "may" and gives a range. That leaves three decisions, each the purchaser's: whether to step at all or hold 385 MPa to rupture; which interval between 8 and 16 hours; and whether the purchase order sets its own increment or interval. A laboratory that chooses after watching the bar survive 100 hours is deciding the loading history of an acceptance test with the result half in view: the wrong party, at the wrong time.
So TCR's reply asked, before testing, for confirmation of the stress to be applied at each step and the interval between increments once the specified duration is completed without rupture. Only then is the test scheduled.
The laboratory follows the loading rule the order invokes, and asks when the order leaves it open.
"A453 Grade 660 stress rupture is an acceptance test, and the specimen is designed to tell you so. The combination bar carries a smooth gauge and a notch under the same load, so if the material is notch sensitive the notch breaks first and the result is a reject, whatever the hours. That is why we settle the step stress and the interval with the purchaser before the furnace is loaded. Once the 100 hours at 650 °C and 385 MPa are passed, every increment becomes part of the record, and that choice has to be theirs, made in advance."
Avinash Tambewagh is Technical Head of TCR Engineering, manages its advanced testing department and has led accelerated creep rupture testing to ASTM E139.
ASTM E139 and ASTM E292: which one governs what
ASTM A453 gives two test methods different jobs. ASTM E139 governs the test; ASTM E292 contributes only the Fig. 1 specimen, and Note 1 says E292's additional data is not determined or reported.
| ASTM E139 | ASTM E292 | |
|---|---|---|
| Scope | Creep, creep-rupture and stress-rupture tests of metallic materials | Time-for-rupture notch tension tests |
| Role under ASTM A453 | The test method (clause 8.2.4.1) | Source of the Fig. 1 specimen only (Note 1) |
| On NABL certificate NABLT0726MH18640 | Yes | Yes, for elongation and reduction in area |
A full ASTM E292 notch tension test is a separate request.
What sits on the NABL scope
Read against the annexure to certificate NABLT0726MH18640 (see quality and accreditation):
| Test | Method | On NABL scope |
|---|---|---|
| Stress rupture, elongation | ASTM E139 | Yes |
| Stress rupture, reduction in area | ASTM E139 | Yes |
| Creep test and creep rupture test | ASTM E139 | Yes |
| Creep rupture test | ISO 204 | Yes |
| Time-for-rupture notch tension test, elongation and reduction in area | ASTM E292 | Yes |
| Stress relaxation of bolting | ASTM E328 | No |
The laboratory tests from 400 °C to 1,100 °C, with applied loads from 1 kN, on six constant-load creep frames rated at 50 kN. Stress relaxation, which governs how a bolt loses preload in service, is a different property and is reported as standard laboratory testing. The companion tension tests on the lot are part of mechanical testing.
What the report should state
A report should let the purchaser's inspector check acceptance without asking a question. It states:
- Identification: grade, class, heat, lot, specimen location and orientation, and the specimen route.
- Loading history: temperature, time at 385 MPa, then each step stress and the time at it.
- Result: total time to rupture, rupture location (smooth section or notch), elongation and reduction in area.
- Statement: conformity against Table 6 and clause 8.2.4.2 or 8.2.4.3, under the decision rule agreed at quotation.
The same discipline runs through TCR's creep rupture testing of SUPER 304H to a BHEL specification.
What an enquiry should carry
The enquiry defines the test before the bar is machined. For A453 bolting serving refining and petrochemicals and power generation, send:
- Specification: the ASTM A453 edition the order cites, and any purchaser requirement beyond clause 8.2.
- Grade and class: Class D needs no stress-rupture test.
- Heat and lot: identification, product form and size.
- Specimens: number, location and orientation, as for the tension specimens.
- Specimen route: combination bar, or separate bars with the purchaser's written approval.
- Step loading: whether used, the stress at each step and the interval.
- Material: an 18 mm × 18 mm × 250 mm blank for each specimen, identified to heat and lot.
Broader bolt and stud validation is covered in NABL accredited fastener testing.
Frequently asked questions
When does ASTM A453 Grade 660 bolting need a stress-rupture test?
Clause 8.2.1 of ASTM A453 requires bolting to meet the stress-rupture requirements of Table 6 for design temperatures above 427 °C. Untested material must be permanently stamped NR. Grade 660 Class D and Grade 668 do not require the test and are stamped NR.
Why does the A453 stress-rupture specimen have a notch?
A bolt thread is a notch, and some alloys lose rupture life at a notch faster than in a plain section. The combination smooth and notched bar exposes that notch sensitivity: clause 8.2.4.2 requires rupture in the smooth section, so a notch failure does not meet the clause.
Does the test stop at 100 hours at 650 °C and 385 MPa?
No. One hundred hours is the minimum time to rupture, and the bar is continued to rupture because rupture location and elongation are part of acceptance. After the minimum, clause 8.2.4.4 permits raising the stress by 34.5 MPa every 8 to 16 hours until it breaks.
Why must the step stress and interval be agreed before testing?
Clause 8.2.4.4 permits step loading but does not require it, and gives a range for the interval. Those choices shape the loading history of an acceptance test, so they belong to the purchaser and are fixed before loading, not decided by the laboratory after the bar survives the minimum.
Is ASTM E139 stress rupture on TCR Engineering's NABL scope?
Yes. Stress rupture to ASTM E139, with elongation and reduction in area as the accredited parameters, is on NABL certificate NABLT0726MH18640 for the Mahape laboratory, as are creep rupture to ISO 204 and notch tension tests to ASTM E292. Stress relaxation to ASTM E328 is not.